A microporous nano insulation board is a rigid panel pressed from fumed silica, an infrared opacifier and a small fraction of reinforcing fibre. Its pores, typically 5–25 nm across, are smaller than the mean free path of air molecules (about 70 nm at atmospheric pressure), so gas conduction and convection inside the panel are largely suppressed. With the opacifier cutting radiant transfer, published supplier curves put thermal conductivity near 0.020 W/m·K at ambient and 0.022–0.023 W/m·K at 200 °C — below still air at roughly 0.026 W/m·K. Density sits at 200–400 kg/m³. SLM supplies this material in two standard grades with continuous-use ratings of 950–1050 °C, plus special grades reaching 1100–1200 °C.
Copper and zinc smelters are among the most demanding places this board can be fitted, and among the easiest to specify wrongly. The reason is simple: the bath runs at 1100–1300 °C, which is hotter than the board itself is rated for, yet the board is never placed against the bath. It belongs on the cold side of a working refractory, where the temperature is far lower. Getting that interface temperature right is the whole job. This guide stays with the product — what its specification means, how to select a grade and thickness, where it is installed zone by zone, how it is protected and inspected, and, most importantly, the positions where a silica-based panel is simply the wrong material. Our application map sets out the same backup position across the other high-temperature industries we supply. What the board is, in specification terms
Read a microporous board datasheet as four linked numbers, not as a single headline conductivity figure.
Conductivity across the temperature range. The value that matters is the one at the board's own mean temperature in service, not the ambient figure. Representative published curves for this material class run approximately 0.020 W/m·K at 20 °C, 0.022–0.023 at 200 °C, 0.025 at 400 °C, 0.028 at 600 °C and 0.033–0.039 at 800 °C (supplier datasheets from several independent producers). Calcium silicate board, by comparison, is quoted around 0.080 at 200 °C and 0.140 at 800 °C; ceramic fibre board around 0.15–0.20 at 800 °C (Promat and Wedge comparison tables). That four-to-fivefold gap at working temperature is the entire commercial case for the panel. How the board is manufactured explains the mechanism in more detail; the datasheet guide shows how to read a curve instead of a single point, and how to check that a quoted figure is a mean-temperature value rather than a room-temperature marketing number. Density and mechanical strength. At 200–400 kg/m³ the board is light, but compressive strength is only about 0.3 MPa at 10 % deformation (supplier datasheets). It is a liner, not a structural component. Specifications must say who supports it — normally the steel shell, a light retaining frame or pins — and must never imply that the panel carries the working lining above it.
Maximum service temperature. Standard grades are commonly rated 1000–1050 °C; extended grades reach 1100 or 1200 °C. This is a limit on the board's own hot face, and it is the number that decides whether a design is viable at all. All grades in this class are Class A1 non-combustible and contain no organic binder, which is relevant in smelter buildings where oil, gas and sulphur-bearing atmospheres coexist.
Facing and format. Boards are supplied as 1000 × 600 mm or similar panels in 10–50 mm thicknesses, sometimes as 25 mm or 50 mm standard items (supplier catalogues). An aluminium-foil or PE-film facing is an option on the product, not a site improvisation. Because the pore network collapses permanently when it takes up water, the facing and the sealed cut edge are part of the specification, not packaging detail. Smelter environments add a second reason: flux dust and sulphur compounds are hygroscopic, and a damp panel in a warm wall loses its performance long before anyone notices a visual defect.
Choosing the grade from the interface temperature, not the bath temperature
Copper and zinc process temperatures are worth knowing, but only because they tell us what the refractory must drop before the board sees it. Published smelter process data put a flash furnace reaction shaft at 1250–1300 °C, matte at 1180–1220 °C and the flash furnace hearth around 1200 °C (EPA AP-42 background report and modern process overviews). Peirce-Smith converters run 1200–1250 °C, with the copper-making stage at 1180–1230 °C. Anode refining furnaces work at 1100–1200 °C. Molten copper in a casting launder is 1080–1300 °C and freezes near 1070 °C. On the zinc side, fluidised-bed roasting runs 900–950 °C, the top of an Imperial Smelting Furnace is held at 1000–1050 °C because the ZnO + CO reduction reverses below about 907 °C, and zinc remelt and casting operate at a much milder 420–480 °C.
None of those numbers is a board rating input. The input is the temperature at the cold face of the working refractory, after 150–300 mm of magnesia-chrome brick, high-alumina castable or silicon carbide has taken the gradient. In practice this means the specifier has to obtain or calculate that interface temperature before selecting a grade, then add a margin for refractory thinning over the campaign. Where the calculated interface sits below roughly 950 °C a standard grade is normally the economical call; where it approaches or exceeds 1000 °C, or where the working lining is expected to wear thin, the extended-temperature grade earns its premium. The SLM-1000 and SLM-1200 comparison sets out that trade-off grade by grade, and the thickness-sizing method gives the layer-by-layer calculation used to arrive at the interface figure in the first place. A common specification error is to size from the bath temperature and conclude that a 1000 °C-rated panel cannot be used in a 1250 °C furnace. The opposite error is worse: assuming that because the bath is hot, any position behind the brick is automatically cool enough. Roof sections, taphole surrounds and launder bottoms run hotter than sidewall averages, and a panel placed there without a thermal check will sinter, shrink and open joints within weeks.
Sizing the layer: what the conductivity curve really buys you
For a flat wall at steady state, heat flux is the temperature difference divided by the sum of the layer resistances plus the outside surface resistance:
q = (T_hot − T_ambient) / ( L₁/k₁ + L₂/k₂ + … + 1/h )
with L in metres, k in W/m·K, and h typically 10–15 W/m²·K for natural convection plus radiation at the outer shell (standard furnace engineering reference). Two consequences follow for this product.
First, the board's advantage is largest where temperature is highest. At 800 °C a microporous panel is quoted at 0.033–0.039 W/m·K against 0.14–0.18 for calcium silicate and 0.15–0.20 for ceramic fibre. A 50 mm microporous layer therefore delivers roughly the same thermal resistance as about 200 mm of calcium silicate at that temperature — consistent with the "up to four times thinner" and "25 mm replaces about 150 mm of ceramic fibre" claims published by producers and furnace engineering consultancies. Those are material-property comparisons, not smelter measurements; we did not find a publicly documented, instrumented copper-converter retrofit giving a measured shell-temperature reduction for a microporous board, so any project-specific saving should be calculated from the actual lining build-up rather than quoted from a brochure.
Second, adding insulation is not free in a smelter. In a launder, patent literature from Outotec (US 7,700,036 / EP 1836015) is explicit: the refractory is deliberately sized so its outer surface runs at 700–900 °C, keeping the 1070 °C copper freezing isotherm inside the refractory. If the external insulation is too effective, molten copper penetrates further into the porous refractory before it freezes, and the launder can leak. This is the single most important sizing rule for the board in copper service — the optimum back-up thickness is a thermal-balance result, not the thinnest layer that minimises heat loss. Cover the launder first, then calculate the wall.
Where space is the driver rather than energy, the same arithmetic works in reverse: a furnace wall can be thinned while holding the same cold-face temperature, freeing internal volume or reducing shell weight. Vendor-reported furnace data claim a 25–40 mm backup layer behind a 150 mm castable lining can pull shell temperature from about 120 °C to below 60 °C; treat that as a manufacturer's figure to be verified on the specific wall, not a guaranteed outcome.
Where the board sits, zone by zone
The useful mental model is one sentence: the board goes behind the refractory, on the cold side, in non-load-bearing, non-wetted, non-abraded positions. Translated onto a copper and zinc plant:
Flash furnace settler sidewalls and uptake non-contact zones. Behind magnesia-chrome or magnesia-spinel brick, where the shell temperature is the target. Reaction shaft and slag-line areas with water-cooled copper jackets are engineered systems; the board is not part of that cooling design.
Converter barrel away from the tuyere zone. Refractory suppliers recommend a designed backup insulation layer in selected non-contact areas to cut shell loss and stabilise the thermal gradient. Tuyere belts, mouths and tapholes see thermal shock, slag attack and mechanical abuse — no panel belongs there.
Anode furnace walls, roof and flue outer layers. Published refractory selections for anode furnaces specify lightweight mullite brick or aluminium-silicate fibre as the outer insulating course; a microporous panel is the thin, high-performance alternative when the shell envelope is constrained.
Launders, troughs and launder covers, between the steel jacket and the refractory flow channel, subject to the freezing-isotherm rule above. The cover is usually the better first investment.
Holding furnaces, casting ladles and ladle lids, as backup behind a high-alumina or silicon carbide working lining. A calcium silicate supplier notes that copper casting at 1100–1250 °C exceeds the rating of its standard 1000 °C board and calls for a 1100 °C-rated product in the backup position — a useful reminder that grade selection is driven by product limits, not by the metal's name.
Zinc roaster shell and ISP upper structure, in the 900–1050 °C envelope, again behind the working lining.
Zinc remelt and holding furnace lids at 420–480 °C. Here the board works thermally but rarely pays for itself; see the boundary section below.
Copper and zinc are not aluminium, and the aluminium furnace guide should not be copied across wholesale. In aluminium service the well-known constraint is that magnesium-bearing alloys reduce silica, so silicon-based linings are excluded from melt contact. Copper presents a different chemistry with the same conclusion: copper oxide fluxes both alumina and silica, which is why silicon carbide is specified for high-wear melt zones (refractory supplier guidance). Installation: moisture, facings, joints and fixings
Four rules govern whether the installed board performs like its datasheet.
Keep it dry from goods-in to heat-up. Water permanently collapses the microporous structure; there is no recovery on drying. Specify foil- or film-faced panels, sealed cut edges and moisture-barrier packaging, and keep pallets under cover. The storage and cutting guide covers handling, cutting tools and same-day edge sealing. On smelter sites, schedule panel fitting after wet castable work and any refractory curing or drying are complete — a freshly washed lining is a common source of avoidable damage. Fit it tight and stagger the seams. A 1 mm open joint in a 20 mm panel can bypass as much heat as several millimetres of solid material, because the gap is a direct radiation and convection path. Butt joints should be tight, staggered between layers, and offset from shell stiffeners and anchor positions. The joint-gap control notes give the tolerances and the inspection method. Do not load it. Retain panels with the shell, pins or a light frame; avoid through-fasteners that crush the panel locally. Where anchors are necessary, detail a compression limiter. Vibration from converters and nearby fans argues for the mechanically reinforced grade rather than the lowest-conductivity grade — a small conductivity penalty is cheaper than a cracked panel.
Protect the hot face. The board must never be the first layer behind flame, slag splash or molten metal. Check the drawing for any location where a taphole, launder lip or burner block could expose an edge. Seal every exposed edge with the facing system, and record the detail on the installation drawing.
QC and acceptance
Incoming inspection should be a short, written gate: verify grade and thickness against the purchase order, check density on a sample, confirm the facing is intact and the pallet wrap unbroken, and require the batch conductivity certificate at the mean temperature relevant to the design. The incoming QC checklist gives the sampling plan and the pass/fail tolerances. After installation, acceptance is thermal rather than visual. An infrared survey of the shell during heat-up and at steady operation will show hot streaks at missed joints, crushed panels and uninsulated anchors far faster than a walkdown. Baseline the shell temperature map at start of campaign and repeat it at planned shutdowns; a rising local reading usually means a joint has opened or a panel has taken moisture. Performance verification describes the measurement points and how to correct for emissivity on a steel shell. When a panel does fail, the failure analysis guide is useful for distinguishing moisture collapse, mechanical crushing and over-temperature sintering — the three look similar on a removed sample but have completely different root causes. Where the board is not the answer
This is the section most often missing from supplier literature, and the one that matters most in non-ferrous plants.
Any position wetted by molten copper, matte, slag or copper oxide. A fumed-silica panel is silica. Copper oxide formed during fire refining dissolves common oxides including alumina and silica, and dense high-velocity copper infiltrates porous ceramics (refractory supplier guidance). Silicon carbide, magnesia-chrome or high-alumina refractories take those zones; the board stays behind them. If a drawing shows the panel within the freeze isotherm of a launder, the design is wrong regardless of how good the thermal numbers look.
A launder where extra insulation has not been thermally balanced. As described above, over-insulating allows copper to penetrate the refractory before freezing and can cause a leak. Covers first, then a calculated backup layer — not a blanket "thinner is better" retrofit.
Any load-bearing, impact or high-velocity-gas position. With roughly 0.3 MPa compressive strength at 10 % deformation, the panel cannot support a working lining, a launder cover walked on by operators, or a taphole surround exposed to slag scouring. Use dense refractory or calcium silicate there and keep the microporous layer in protected backup zones only.
Unsealed wet or wash-down environments. Without a facing and sealed edges, a single wet shift can destroy the pore structure. Where regular wash-down is unavoidable, either detail a fully encapsulated panel with a drained outer skin or choose a different material.
Low-temperature zinc duties. Zinc remelt at 420–480 °C, zinc electrowinning electrolyte at 60–80 °C, and the cold-chain and ambient equipment around a plant do not justify a 1000 °C-grade panel. Conventional insulation is cheaper for the hot-end duty, and evacuated panels are the correct technology near ambient — the cold-chain VIP comparison explains that boundary. Specifying a high-temperature board in those positions is not a technical error so much as a commercial one, and it is worth saying so plainly in an RFQ response. Hot faces above the grade rating. Where the calculated cold-face temperature approaches the grade ceiling, or where refractory wear will push it there over the campaign, move to the extended grade or add a sacrificial fibre course. A panel run above its limit shrinks and opens joints; no amount of extra thickness compensates for a exceeded temperature rating.
Procurement, packaging and shipping
A workable purchase order names four things together: grade and maximum service temperature, thickness, facing, and a cut list tied to an approved drawing. Add the batch conductivity certificate, the density tolerance and the moisture-barrier packaging requirement in the same line items, so a cheaper quotation cannot quietly drop them. If the design uses two grades — standard on most walls, extended near tapholes — call them out separately with a marking scheme; mixed pallets are a predictable installation error. For the product itself, see the high-strength nano insulation boards page for the grade and format range. Because the panels are brittle and moisture-sensitive, packaging is part of the product, not a freight afterthought. Panels ship flat on pallets, sealed in moisture-barrier film, with corner protection and no other cargo stacked on top. Container loading notes cover palletising, desiccant, weather protection during port dwell, and how to keep panels dry through an overseas smelter project. Ask the supplier to state the packaging specification on the quotation; comparing unit prices without it is misleading. For a first enquiry, include the lining build-up (refractory type and thickness), the bath and calculated interface temperatures, the target shell temperature, available backup thickness, and whether the position is exposed to wash-down or vibration. Those five inputs let the grade and thickness be proposed on engineering grounds rather than by product name alone.
Frequently asked questions
Can the board be used directly against molten copper? No. It is silica-based, and copper oxide attacks silica and alumina. It belongs behind a silicon carbide, magnesia-chrome or high-alumina working lining, on the cold side.
Is 1200 °C bath temperature a problem for a 1000 °C-rated board? Not by itself. The relevant temperature is the cold face of the working refractory. Calculate or measure it, add a margin for lining wear, then choose the grade.
Why not simply use the thinnest possible backup layer in a launder? Because the refractory must stay hot enough on its outer face (700–900 °C in the patent literature) to keep the copper freezing isotherm inside the refractory. Over-insulation can drive copper penetration and leaks.
How thin can the layer be? Typical panels are 10–50 mm, with 25–40 mm common in furnace backup positions. The final thickness comes from the resistance calculation and the freeze-isotherm constraint, not from a catalogue minimum.
What is the most common field failure? Moisture, followed by crushed panels and open joints. All three are installation and handling issues, and all three show up first as a local hot streak on an infrared shell survey.
Does zinc service need the extended grade? Usually not. Roasting at 900–950 °C is within a standard grade's range when the panel is correctly placed behind refractory; remelt at 420–480 °C seldom justifies a high-temperature panel at all.
Bottom line
Microporous insulation board earns its place in copper and zinc smelting as a thin, low-conductivity backup layer that cuts shell loss and frees space inside a fixed shell envelope. Its value comes from a conductivity curve that stays flat while conventional materials climb, and its risk comes from the same place: a very effective insulator can move a freezing isotherm, and a silica-based panel cannot survive melt exposure. Specify from the calculated interface temperature, keep the board behind the refractory, seal it against moisture, stagger the joints, verify with an infrared survey — and decline the positions where the chemistry or the heat balance says no.
Nano insulation boards are supplied by SLM (Nantong Suleiman) in two standard grades with extended-temperature options. Figures marked "supplier datasheets" are published values for this material class; process temperatures are from published smelter process data, EPA AP-42 and equipment literature; launder thermal-balance figures are from Outotec patent literature; chemical compatibility guidance is from refractory suppliers. We did not find a publicly documented instrumented copper-smelter case study quantifying shell-temperature reduction for a microporous retrofit. Confirm all grades, facings and dimensions against the current SLM datasheet before specification.