Hot metal leaves the blast furnace around 1400–1450 °C and arrives at the converter cooler. A torpedo ladle car is the vessel that carries it, and published plant figures put in-service shell temperatures above 250 °C, rising to about 350 °C late in a campaign. Lining thermal storage is reported to account for 45–50 % of total heat loss, wall losses about 20 %, and open-surface radiation another 20–30 %. Those numbers describe the vessel, not our product. Our application map places SLM-1000/1200 microporous insulation board on the cold side of a dense permanent lining, between that lining and the steel shell, and nowhere else. This is a product guide: what the board is, what its conductivity means at the temperatures a backup layer actually sees, how to read shrinkage and classification figures, how to choose grade, facing and thickness from the permanent-lining cold face, where it fits in a torpedo ladle build-up, how to cut, fix, dry and inspect it, and where the material is the wrong answer. One honest limit up front: apart from one steelmaker's own published technical report, no independent or peer-reviewed field measurement of microporous board in a torpedo ladle was found, and no public measurement of vibration effects or lining-life extension was found.
What the board is, and what it is not
The board is a pressed composite of fumed silica, reinforcing fibre and an opacifier. Pores smaller than the mean free path of air suppress gas conduction and convection, while the opacifier scatters the infrared radiation that dominates above 400 °C. How the board is manufactured explains the difference from a fibre blanket: no fibrous network to settle under railway vibration, no organic binder to burn out, no open cell for slag vapour to circulate through. Commercial grades carry 1000, 1100 and 1200 °C classification temperatures. One-hand datasheets give densities near 240–450 kg/m³, compressive strengths from 0.12 to just over 1 MPa, and thicknesses from 3 to 50 mm; steel-industry products are commonly supplied at 5, 7 or 10 mm. Facings include E-glass cloth, PE film, aluminium foil, mica laminate and hydrophobic cores. Panels can be cut, sawn, drilled and punched to a relining drawing. A1 non-combustibility is a material property, not a fire-protection rating, and this product is a thermal backup layer rather than a safety device.
The product boundary follows from that. A cold-face board is not a working lining, not a safety or penetration barrier, not a structural layer, and not a substitute for a ladle lid. Datasheets for microporous granulate state plainly that liquids — water, oil, petroleum spirit — densify the pore structure and change its conductivity, while non-condensed moisture does not. Facing, edge sealing and packaging are therefore part of the specification, not packaging detail.
Product conductivity at backup temperatures
Published SLM curves give roughly 0.020 W/m·K at 20 °C, 0.022 at 200 °C, 0.025 at 400 °C and 0.033 at 800 °C. Independent commercial datasheets sit in the same band. MICROTHERM PANEL 1000R lists 0.023 / 0.026 / 0.031 / 0.039 W/m·K at 200 / 400 / 600 / 800 °C; a steel-grade 1000 product lists 0.023 / 0.026 / 0.030 / 0.036; a 1200-grade panel 0.029 / 0.033 / 0.039 / 0.044. The datasheet guide explains how to read these as mean-temperature values tied to a test method, a density and a defined grade before putting them into a calculation. | Mean temperature | Microporous board | Ceramic-fibre blanket | Calcium silicate | Insulating firebrick | |---|---|---|---|---| | 200 °C | 0.022–0.023 W/m·K | ~0.06–0.07 W/m·K | ~0.06–0.10 W/m·K (room temp) | — | | 400 °C | 0.025–0.027 W/m·K | ~0.10–0.12 W/m·K | ~0.10 W/m·K | ~0.14–0.19 W/m·K | | 600 °C | ~0.029–0.034 W/m·K | ~0.17–0.22 W/m·K | ~0.12 W/m·K | ~0.16–0.23 W/m·K | | 800 °C | 0.033–0.044 W/m·K | ~0.19–0.30 W/m·K | ~0.12–0.15 W/m·K | ~0.18–0.31 W/m·K |
These comparison values come from supplier datasheets and an environmental product declaration, not one comparative test programme. Lightweight castable is quoted near 0.28–0.58 W/m·K at 400–600 °C. The board's curve stays nearly flat while fibrous and calcium-silicate alternatives steepen, which is why a millimetre-scale layer can replace tens of millimetres of conventional backup. Above about 600 °C radiation through the pores grows, so the grade's opacifier and the hottest interface temperature matter more than the room-temperature figure.
Reading the datasheet before selecting the board
Classification temperature is a short shrinkage test, not a continuous working limit. EN 1094-1 states that it does not imply continuous usability at that temperature; for amorphous high-temperature insulation wools the continuous figure is typically 100–150 °C lower. That single distinction belongs in a purchase order here, because a torpedo ladle runs hot for hundreds of cycles between relinings.
Shrinkage is equally conditional. One datasheet quotes less than 0.5 % after a 12-hour single-face soak at 1000 °C but less than 3 % after a 24-hour full soak at the same temperature; another gives 0.6 % versus 3.0 % at 1050 °C. A five- to six-fold difference hides in the test condition. Ask for the figure with soak type, temperature and duration written on the certificate.
Also check what the grade actually is. Steel-grade 1200 products and some 1050 °C boards are alumina-based or contain zirconium silicate rather than pure fumed silica, and well-known "SILCA" lines are largely calcium silicate, a different material. Request the current conductivity curve, density, compressive strength, thickness tolerance, facing type and written confirmation of the continuous service temperature.
Selecting the board from the permanent-lining cold face
A 1450 °C bath does not expose a backup panel to 1450 °C. What the panel sees is the cold face of the permanent or safety lining in front of it. One published finite-element study of a 285 t car reports layer temperatures of about 1150 °C at the hot-face boundary, 1054 °C, 820 °C, 477 °C and then roughly 131–135 °C near the shell — a model result, not an in-service infrared reading. Plant reports of 250–350 °C shell temperatures use a different measurement basis; the two figures must not be mixed in one calculation.
Grade is chosen from the worst case at the board's own interface, not from hot-metal temperature. The SLM-1000 and SLM-1200 comparison sets out where a higher grade pays. In a torpedo car the excursion case dominates: a thinned working lining, a delayed relining and a long hot hold all raise the permanent-lining cold face together. Ask for shrinkage at that interface temperature with the soak condition stated, and add margin for the late-campaign condition rather than the new-lining condition. Thickness follows from allowable shell heat flux. The thickness-sizing method guide gives the full one-dimensional calculation. An illustrative example: assume a 350 °C permanent-lining cold face, a 200 °C shell target and 300 W/m² allowed by the vessel designer. Required resistance is (350 − 200) / 300 = 0.50 m²·K/W. At a mean board conductivity near 0.030 W/m·K that is about 17 mm of board, against roughly 50 mm of calcium silicate at 0.10 or 65 mm of fibre blanket at 0.13. Those inputs are design assumptions, not measured car values; no public shell heat-flux limit for a torpedo ladle was found. The useful output is often not total lining thickness but usable vessel volume. Suppliers claim a thin backup frees several per cent of capacity, and a published lining study notes that a worn working layer was almost half its design thickness. Both are geometry arguments to check against the vessel drawing, not a licence to thin the working lining or move the penetration isotherm outward.
Where the board sits in a torpedo ladle build-up
Published lining sections describe, from the hot side inward, an Al₂O₃-SiC-C working lining zoned for roof, slag line, metal zone and impact area, a ramming or permanent layer, a pyrophyllite or insulating brick course, and the steel shell. One Chinese plant description lists a low-cement castable permanent layer plus clay insulating brick; a 285 t study gives a 130–140 mm working layer, 40 mm ramming material and 35 mm pyrophyllite brick.
Read as a product rule: the board is a candidate only for the backup position between that insulating or permanent course and the shell along the barrel. It replaces part of the conventional insulating brick or calcium silicate thickness. It does not replace the permanent layer, whose job includes stopping metal and slag that penetrate brick joints, and it does not go into the working lining, the throat, the slag line or the impact area.
This is the same cold-face discipline used in steel ladles, holding furnaces and other vessels in our range. A dense, chemically resistant layer faces the process; the board works on the cold side of it and is protected by it. Where a monolithic permanent layer is cast in place, the board belongs on the shell side of that layer so it never sees free water from the castable.
What the published measurement means for the board
One steelmaker's technical report describes a torpedo car with a 3 mm microporous layer installed between the steel shell and the permanent refractory, confirming approximately a 50 °C lower steel-shell temperature and a 25 % reduction of radiant heat loss. The same report gives 5 mm in a hot-metal ladle producing a 96 °C shell-temperature drop and 45 % less heat loss, and a monolithic ladle with the board kept on the dry side of the permanent layer showing 70 °C and 36 %. These are plant results published by the steelmaker, not an independent comparative trial, and the report does not state hot-metal temperature retention or campaign life.
That distinction matters because most other numbers in circulation are supplier claims. Vendor pages quote 50 t ladles falling from 370 °C to 240 °C, 130 t ladles dropping 80–100 °C, roughly 40 °C hotter metal at the converter and about 5 % more volume. None of those carries a stated measurement protocol, car identity or third-party verification. The ROI calculation used for steel ladles can be adapted to a car fleet, but its inputs must be the measured shell survey and the real tap-to-converter temperature drop, not a marketing percentage. An academic consortium's in-situ ladle measurements add a useful product-side datum: a 5 mm board produced a 400 °C temperature drop across the near-shell region, and the bake-out showed two moisture plateaus near 100 °C and 240 °C. A late-1990s journal study comparing infrared shell surveys with a thermal model found deviations up to 45 K on basic linings, attributed to ageing of the microporous layer — shrinkage, carbon deposits and particle growth raising conductivity — and recommended a maximum service duration. Together these say the board works, and that its performance is not constant forever.
Why the throat, slag line and impact zone are excluded
The working lining wears unevenly. Published damage studies describe metal and slag penetration through brick joints, skull formation at long residence times and low metal temperatures, spalling across the 1550–1650 °C tapping to 800–1200 °C empty-car cycle, and calcium-aluminate formation where high-basicity desulfurisation slag meets aluminosilicate brick. One plant reports about 0.5 mm of working-lining loss per fill and a first intermediate repair near 85 fills.
A board behind a cracked or thinned working lining at those positions would see metal, slag or temperatures far above its rating. Silica is not chemically stable against molten alkali and metal oxides, and no dedicated compatibility study between fumed-silica board and hot metal or desulfurisation slag was found. The engineering answer is to keep a dense permanent layer in front of the board and to exclude the throat, slag line and impact zone from the board layout entirely, even if the shell there is hottest.
Vibration is a second, separate limit. Torpedo cars run on rail at a few kilometres per hour loaded and tilt for pouring; lining suppliers warn against mechanical compression and recommend staggered, non-through joints. No public measurement of microporous-board behaviour under transport vibration or impact was found. That is a reason to design the fixing conservatively and to inspect at the first intermediate repair, not a reason to assume the board is unaffected.
Installing the board: bake-out, joints, fixing and moisture
Before any panel is ordered, re-check the preheat and dry-out curve for the vessel. One published baking schedule runs about 45–48 hours through staged holds near 310 °C, 590 °C and 990 °C, with brick joints held to 2 mm; older practice took roughly twice as long. Free water and chemically bound water leave at different plateaus, and a sealed, foil-faced panel on the wrong side of a wet castable can trap that water. A general installation guide for ladles covers the sequence; the car-specific drawing governs where panels start and stop. Joints decide much of the result. A narrow open seam through a 17 mm panel bypasses the pore structure and behaves as a thermal bridge. Fit panels tight, stagger joints between courses, avoid continuous vertical seams, pack residual gaps with compatible fibre and allow 1–2 mm for expansion at steel interfaces. The joint-gap control notes give the tolerances and packing detail; cone ends, trunnion areas and shell returns are where curved, pre-cut pieces earn their cost. Fixing needs its own check. Datasheets allow glue, anchors, pins and clips, but a fastener driven from the shell into the permanent layer becomes a heat path and a corrosion site, and an over-tightened clamp crushes a panel whose compressive strength is below 1 MPa. Where the shell detail cannot be adapted, retain panels with a light cold-side frame. Never use the board to close an expansion gap that was designed to move.
Moisture control is unforgiving. Panels arrive in sealed moisture-barrier packaging, are stored flat and dry off the floor, and are cut only when ready to fit. Storage and cutting guidance covers the handling sequence; wetted panels are rejected, not dried and reused. Every cut edge is sealed the day it is cut. Water-repellent facings exist specifically for castables and mortars, but hydrophobic treatments have their own temperature limits and degrade after first heating in some product lines. Inspection, acceptance and what a survey can prove
The incoming QC checklist covers dimensional tolerance, thickness uniformity, density, facing integrity, edge sealing, package moisture indication and certificates against the order. For a car add three items: the shrinkage figure with its soak condition, written confirmation of the continuous service temperature at the design interface, and the calculated interface temperature in the agreed lining build-up. The meaningful acceptance test is a like-for-like shell-temperature and heat-flux survey at defined points around the barrel, logged with hot-metal temperature, fill count, residence time, ambient conditions, lid use and campaign age. Performance verification guidance describes the instrumented approach. A reading taken on a different car, in a different season or with the lid off is not comparable; published models show slag thickness, lid and wind speed all changing temperature drop. A local hot area usually means a gap, a displaced panel, a failed edge seal or a crack in the permanent layer in front of it — moisture and crushing are the two classic ways this material loses its pore structure — and rarely insufficient thickness. Record the survey as the baseline for trending through the campaign, and re-measure at the first intermediate repair. If shell temperature climbs late in the campaign, treat it as a lining-condition signal first and a board-ageing question second.
Where the board is not the answer
The throat, slag line and impact zone. Working-lining wear, metal and slag penetration and tapping shocks can reach the cold face there. A silica-rich panel must not be the last line of defence.
The hot face and the working lining. 1400–1450 °C iron and high-basicity desulfurisation slag are outside the board's rating and chemical capability.
The permanent or safety lining. That layer stops penetration and carries the consequences of a brick-joint failure. A porous panel cannot substitute for it, and no compatibility study supports that position.
The wet side of a castable. Free water from monolithic permanent layers destroys the pore structure permanently. Keep the board on the dry, shell side and provide a drainage path during bake-out.
Load-bearing and clamped positions. At under about 1 MPa compressive strength the board cannot carry the lining, the trunnion loads or maintenance traffic, and it must not be compressed to close a fit.
The open top. Published studies credit a ladle lid with 1.1–2.2 °C/h slower cooling and roughly 19 °C higher metal after a long hold. Surface radiation is a lid problem; a shell-side board does not fix it.
Excursions above the continuous rating. Selecting from average bath temperature or a new lining invites shrinkage, opened joints and hot spots late in the campaign.
Unverified ageing and vibration claims. No public measurement of board behaviour under railway vibration, or independent evidence of lining-life extension, was found. Treat both as inspection items, not promised benefits.
Buying the board: RFQ inputs and packaging
Specify grade, thickness, facing, panel dimensions and cut list together, and call out sealed moisture-barrier packaging, edge-sealing material and the shrinkage test condition. Ask for the current datasheet with its conductivity curve and written confirmation of the continuous service temperature at the design interface. High-strength nano insulation boards are listed on the SLM product page; use that as the quotation reference so conductivity is compared at the same mean temperature and density. A workable RFQ states car capacity, the full lining section with every layer thickness, hot-metal temperature at tap and at the converter, transport distance and residence time, fills per campaign and relining window, whether in-car desulfurisation is practised, throat/slag-line/impact-zone exclusion zones, measured shell-temperature baseline, lid practice and allowable shell heat flux. Without the lining drawing and a shell baseline, a thickness recommendation is a guess.
Panels ship flat on pallets, are brittle and moisture-sensitive, and are usually needed inside a short relining window. Packaging, weather protection and the delivery date are part of the price comparison. Container loading notes cover palletising and keeping panels dry through an overseas project and site lay-down. Frequently asked questions
Can the board be fitted behind the throat or slag line? No. Those positions lose working lining first and can expose the cold face to metal, slag and temperatures beyond the board's rating. Exclude them from the panel layout.
How is thickness chosen? From the permanent-lining cold face, the target shell temperature and the allowable heat flux. The worked example gives about 17 mm for a 0.50 m²·K/W requirement, with all inputs stated as design assumptions.
Is there published field evidence? One steelmaker's technical report gives about 50 °C lower shell temperature and 25 % less radiant heat loss with a 3 mm layer. No independent peer-reviewed trial, hot-metal temperature-retention result or lining-life measurement was found.
What changes during bake-out? The preheat schedule must let free and bound water escape through the permanent layer. Keep the board on the dry side of any wet castable, seal every cut edge and re-check the curve before commissioning.
How is a failing installation detected? By a shell-temperature and heat-flux survey at fixed points, trended against fill count and campaign age. A new hot spot usually means a joint, a fixing or a crack in the layer in front of the panel.
Bottom line
Microporous insulation board earns its place in a torpedo ladle by delivering large thermal resistance in a few millimetres at the one position where extra resistance is wanted: the cold side of a dense permanent lining along the barrel. It can cut shell heat loss and free lining thickness, and one published steelmaker trial supports that with measured numbers. It does not face hot metal, replace a safety lining, tolerate water, carry load, close the open top or belong behind a slag line that wears through. Specify it from the worst-case interface temperature, keep it on the dry side of castables, control joints and fixings, and verify with a like-for-like shell survey through the campaign. Where chemistry, wear, load or vibration can reach the board, choose a different material.
Data levels: hot-metal temperature, shell temperatures, lining build-ups, temperature-drop and lidding studies, baking schedules, campaign counts and damage mechanisms from steel-industry plant reports, peer-reviewed papers, patents and conference literature; conductivity, density, strength, classification temperature definitions, shrinkage conditions, facings and liquid sensitivity from commercial microporous insulation datasheets, with SLM values from our own current datasheet; the 3 mm car result from a steelmaker's published technical report, not an independent trial; the 400 °C near-shell drop and moisture plateaus from an academic consortium's in-situ ladle measurements; the ageing/model deviation from a 1998 journal study. Supplier-quoted shell-temperature, capacity and hot-metal gains are manufacturer claims without a stated measurement protocol. Comparison conductivity values for fibre, calcium silicate, insulating brick and castable come from supplier datasheets and an EPD. The resistance calculation is a one-dimensional steady-state estimate with its assumptions stated. No public independent measurement of a microporous-board retrofit on a torpedo ladle, no public study of vibration effects, and no independent lining-life result was found. Confirm all product values against the current SLM datasheet before specification.